EPDM compounds range from 500–2,500 psi tensile strength and 100–700% elongation at break [S1][S2].
The grade matters: a 40 Shore A E1022 compound tests at 8.5 MPa (1,225 psi) and 660% elongation, while RC0329 at 50 Shore A specifies 8 N/mm² and 500% [S3][S4].
EPDM Property Ranges and Grade Meaning
EPDM is not a single fixed mechanical specification. General selection tables place hardness at 30–90 Shore A, tensile strength at 500–2,500 psi, and elongation at break at 100–700% [S1][S2].
Those values are screening limits, not guaranteed properties for every compound. Grade selection must consider hardness, formulation, cure system, filler content, test method, specimen geometry, and aging environment [S1][S3]. For material identification, EPDM rubber is normally used interchangeably with ethylene propylene rubber, EP, EPR, and EPT, while ASTM D2000 classifications include AA, BA, CA, and DA [S1][S2].
Published Grade Data for Direct Comparison
Four disclosed EPDM grades show why tensile strength and elongation cannot be treated as interchangeable measures. Marco E1022 is a black, sulfur-cured 40-durometer EPDM compound with an ASTM D2000 specification of M2BA407 A14 B13 F19 and a service temperature of -50°F to 300°F (-45°C to 150°C) [S3].
RC0329 is a premium soft EPDM sheeting at 50±5 Shore A, density 1.05 g/cm², tensile strength 8 N/mm², and elongation at break of 500% [S4]. The Trygonal EPDM standard records 11.7 MPa tensile strength and 263% elongation at break under DIN 53504, plus compression set of 28% at 23°C for 70 hours and 24% at 70°C for 22 hours [S6].
Strength, Elongation, and Hardness Are Different Decisions

Higher tensile strength does not guarantee higher elongation, and neither property establishes service life by itself. The Trygonal standard combines 11.7 MPa tensile strength with 263% elongation [S6]. RC0329 sits between those elongation values at 500% and specifies 8 N/mm² tensile strength [S4].
On a criteria basis, compare grades by tensile strength for resistance to tensile rupture, elongation for deformation before break, and hardness for stiffness and sealing contact. Use compression set as a separate criterion for sustained sealing, especially at elevated temperature. This matters because EPDM compounds can have good abrasion and flex-cracking resistance while still delivering only fair-to-good tear resistance and rebound [S1][S2].
The 50 Shore A RC0329 grade is intended for sheeting, gaskets, and weather-resistant components, with a -40°C to +100°C working range and no cracks after 48 hours of ozone exposure at 40°C [S4]. E1022 specifies a service-temperature range of -50°F to 300°F (-45°C to 150°C) [S3].
Where EPDM Grade Performance Fits
EPDM suits outdoor weather seals, potable-water gaskets, steam service, electrical insulation, and components exposed to ozone, sunlight, water, acids, or alkalies [S2][S5]. These applications reward weather resistance, steam resistance, and oxidation resistance more than petroleum-oil resistance. For exposed rooftop and water-system applications, the compound-selection logic in Specify EPDM for autoclave and steam service remains separate from the tensile-strength decision.
The candidate grades support several specific use cases. E1022 is a sulfur-cured EPDM compound with good heat and compression resistance and resistance to ketones, hot and cold water, steam, alkalis, polar solvents, ozone, sunlight, alcohols, glycol engine coolant, and Skydrol phosphate ester hydraulic fluid [S3].
RC0329 supports gasket, strip, and sheet applications where a tensile strength of 8 N/mm², elongation of 500%, and 25% compression set after 22 hours at 70°C are required by the product specification [S4]. Its heat-aging data show a 10% reduction in tensile strength and a 30% reduction in elongation at break, while compression set rises to 45% after 22 hours at 100°C [S4].
Chemical and Thermal Limits That Qualify the Numbers

Do not select EPDM from tensile and elongation data alone when the part contacts petroleum products. General EPDM guidance rates oil, gasoline, aliphatic and aromatic hydrocarbon fuels, and halogenated solvents as poor matches [S1][S2]. E1022 is specifically not recommended for oils, gasoline, kerosene, petroleum oils, hydrocarbon fuels, and halogenated solvents, although it resists ketones, hot and cold water, steam, alkalies, ozone, sunlight, alcohols, glycol engine coolant, and phosphate-ester hydraulic fluid [S3].
Temperature changes the usable mechanical properties. RC0329, tested to DIN 53508, recorded a +5 Shore A hardness change, -10% tensile-strength change, and -30% elongation change after heat aging [S4].
Compression set remains the more discriminating sealing metric at elevated temperature. RC0329 specifies 25% after 22 hours at 70°C and 45% after 22 hours at 100°C under DIN ISO 815, while E1022 records 11% permanent set after 22 hours at 70°C under ASTM D395 Method B [S3][S4]. Different test methods and conditions prevent direct ranking without a common test plan.
Procurement Data to Require Before Ordering
Require the grade, hardness tolerance, tensile-strength test method, elongation-at-break method, cure system, and service-fluid exposure before comparing supplier figures. E1022 identifies ASTM D2000 M2BA407 A14 B13 F19, sulfur cure, black color, and a 40±5 Shore A specification; its typical results are 44 Shore A, 1,225 psi, and 660% elongation [S3].
For sheeting, RC0329 adds a product code, density of 1.05 g/cm³, sheet thicknesses from 1 mm to 40 mm, and a 50±5 Shore A tolerance [S4]. These identifiers prevent a generic “EPDM” label from substituting for the actual material grade. For a wider comparison between EPDM and alternative elastomer families, engineering plastic provides context for why tensile strength alone cannot decide elastomer compatibility.
Before releasing a component, verify the grade-specific datasheet against the service temperature, compression condition, chemical exposure, and required elongation. A defensible selection records at least the tensile strength, elongation at break, hardness, compression set, and applicable test method, then distinguishes laboratory values from guaranteed purchase requirements.