Cement Loss on Ignition: Meaning, Limits, and Testing

Table of Contents
  1. What Cement LOI Measures
  2. The 3% Cement LOI Limit
  3. How the LOI Measurement Is Performed
  4. High LOI and Its Practical Consequences
  5. LOI for Kiln-Processed Materials
  6. Method Selection and Accuracy Controls
  7. Decision Rules for Engineers
Cement Loss on Ignition: Meaning, Limits, and Testing

Cement loss on ignition is the percentage of sample mass lost when ignited at 900–1000 °C, with volatile material released during heating.

The result detects moisture, carbon dioxide, and organic or other volatile constituents, so it serves as a quality and composition check rather than a direct measurement of cement strength [S3][S4].

What Cement LOI Measures

Loss on ignition compares the initial cement mass with the mass remaining after high-temperature heating. The calculation is expressed as the mass lost divided by the initial sample mass, multiplied by 100; test guidance describes the result as a percentage of the original sample [S3][S4].

A few grams of cement are tested in a tared, pre-ignited crucible. Published cement procedures use approximately 1–10 g of sample, heat it to 900–1000 °C for 15 minutes, cool it in a desiccator, and reweigh it [S3][S4].

The mass difference is not a single identified substance. It can include moisture, carbon dioxide released from carbonates, and organic compounds, while the broader LOI method also identifies volatile constituents through their disappearance during ignition [S1][S3]. For clinker and finished cement, an elevated product LOI can also indicate that pyroprocessing was incomplete, leaving unburnt material in the product [S1].

The 3% Cement LOI Limit

It does not replace compressive-strength testing, soundness testing, setting-time testing, or chemical analysis [S3][S4].

The applicable limit depends on the material and the governing product standard. ASTM C618 addresses coal ash used in concrete, and the source material states that ASTM C618 specifies a maximum LOI of 6 wt% for Class C and Class F coal ash while being used in concrete, although recent studies have questioned this limit [S7][S2].

How the LOI Measurement Is Performed

The operational sequence requires a calibrated balance, a tared crucible, controlled heating to 900–1000 °C, controlled cooling, and a second mass determination [S1][S3][S4].

The calculation is normally arranged as:

<strong>LOI (%) = [(initial sample mass − final sample mass) ÷ initial sample mass] × 100</strong> [S3][S4].

Mass stabilization is central to the method. The sample is heated until its mass ceases to change, with the process repeated where necessary to demonstrate completion [S1]. The 15-minute hold and 900–1000 °C range cited for cement testing provide a defined operational basis for releasing the volatile components [S3][S4].

Thermogravimetric analysis provides a variant in which mass change is monitored as temperature changes [S1]. Traditional furnace LOI determines total mass loss after heating a sample to a temperature as high as 1,000 °C, while automated split LOI analysis was introduced on 2026-04-07 to streamline cement testing workflows [S5].

High LOI and Its Practical Consequences

High-LOI fly ash can influence concrete work, setting, and early-age performance, so the meaning of the LOI limit depends on whether the material is cement, clinker, fly ash, limestone, lime, or another mineral product [S1][S2].

In a high-volume fly-ash concrete study, ashes with LOI values of 5% and 8% were compared at fly-ash replacements of 0%, 20%, 40%, 50%, 60%, and 80% by mass of total cementitious materials. Concrete containing 8% LOI ash remained usable for structural concrete up to a 60% replacement level, although fresh and hardened properties were inferior to those made with 5% LOI ash [S2].

Higher replacement levels produced longer setting times. The 8% LOI mixtures also showed lower fresh and hardened properties than the 5% LOI mixtures, although the study identified adequate strength development through 365 days, high modulus of elasticity, and low dry shrinkage relative to a control concrete with 28-day compressive strength of 30 MPa [S2].

They show why a numerical limit must be applied to the correct material and why a single LOI value does not describe every concrete performance consequence [S2][S3].

LOI for Kiln-Processed Materials

For pyroprocessed raw materials, LOI is approximately equivalent to the mass loss that the material will experience in a kiln [S1]. This makes it a practical proxy for comparing kiln-feed calcination behavior and for checking whether the finished product experienced complete thermal processing.

The test covers several material groups, including limestone, lime, calcined bauxite, refractories, and cement, each with its own procedure and acceptance criterion [S1]. In finished cement, a high LOI can point toward incomplete pyroprocessing; in limestone and lime, the result may reflect decomposition of carbonates and loss of combined water [S1].

This kiln relationship also explains why LOI is not simply a moisture test. Although free moisture can contribute to the measured loss, the 900–1000 °C treatment drives off multiple volatile constituents, so a low result requires controlled sampling, dry handling, and proper cooling before weighing [S1][S3].

Method Selection and Accuracy Controls

Muffle-furnace LOI measures total mass loss after high-temperature ignition, while thermogravimetric analysis can record mass change as a function of temperature, offering a more detailed thermal profile [S1][S5].

For routine cement acceptance testing, the furnace method is straightforward: weigh the crucible, add 1–10 g of cement, heat to 900–1000 °C for 15 minutes, cool in a desiccator, and determine the final mass [S3][S4]. For process diagnosis, TGA can help separate mass-loss events across a temperature program, whereas split analysis can reduce the manual workload in cement-testing operations [S1][S5].

Accuracy depends on controls that are easy to lose in day-to-day use. The balance must be calibrated, the crucible must be clean and pre-ignited, the selected furnace temperature must be maintained consistently, and the sample must cool without absorbing atmospheric moisture [S1][S3][S4]. Multiple determinations and a mean result are recommended to identify anomalous measurements or inconsistencies [S3][S4].

Decision Rules for Engineers

Cement LOI is used as part of general-use Portland cement quality and composition assessment, but acceptance also requires correct sampling, method compliance, and the applicable product standard [S3][S4].

Use the value first to identify excess volatile material or incomplete processing, not as a substitute for strength testing. Rising LOI between production lots can prompt checks of kiln stability, product cooling, moisture ingress, sample handling, and laboratory repeatability before a quality decision is made [S1][S3][S5].

For fly ash, do not import a cement limit blindly. The applicable limit depends on the coal ash class and governing standard, while concrete performance can still vary between ash lots with 5% and 8% LOI [S2][S7].

LOI can reflect multiple volatile constituents, including moisture, carbon dioxide, and organic substances [S3][S4].

Frequently asked questions

At what temperature and sample hold time is cement typically tested for loss on ignition?

Published cement procedures heat approximately 1–10 g of cement at 900–1000 °C for 15 minutes. The sample is then cooled in a desiccator and reweighed to determine mass loss.

How is cement loss on ignition calculated?

LOI is calculated as [(initial sample mass − final sample mass) ÷ initial sample mass] × 100. The result represents the percentage of the original sample mass lost during ignition.

Does an 8% LOI fly ash comply with the ASTM C150 cement limit?

ASTM C618 permits up to 6 wt% LOI for Class C and Class F coal ash used in concrete.

7 sources
  1. Loss on ignition
  2. Effects of the Loss on Ignition of Fly Ash on the Properties ...
  3. Measuring Loss on Ignition in Cement with TGA (Oct 28, 2026)
  4. Using a TGA Machine to Measure LOI in Cement
  5. Streamline Cement Testing with Automated Split LOI Analysis (Apr 10, 2026)
  6. Loss on Ignition (LOI) Testing
  7. Reliability of Loss on Ignition (LOI) Test for Determining the ...