Solid EPDM flange gaskets are normally installed at 25–40% compression, with a practical minimum of 10–15% and an upper limit near 50% [S3].
FKM is the stronger choice for elevated-temperature and aggressive chemical service, but its sealing performance still depends on sustained bolt load, compression, flange finish, and resistance to creep relaxation.
EPDM Relaxation Under Sustained Flange Load
EPDM relaxation is the time-dependent reduction in gasket thickness and contact stress after the flange load has been applied. Heat increases relaxation and reduces the residual bolt load acting through the gasket, while pressure cycling can make a previously effective joint weep [S4].
This behavior is distinct from installation compression. Compression percentage is calculated as [(T_free − T_compressed) / T_free] × 100, so a 3.0 mm gasket compressed to 2.1 mm has 30% compression [S3]. Compression percentage is a geometry and installation parameter rather than a material property, and solid EPDM design targets typically fall in the 25–40% range [S3].
The practical consequence is that initial gasket contact stress is not the same as sealing stress after months at temperature. Elastomeric gasket compounds can maintain recovery when their compression set is low, but the joint still depends on adequate residual flange load and an even bolt pattern. A normal, symmetric bolt pattern distributes load across the gasket ring; an irregular pattern is more susceptible to leakage [S7].
For EPDM, design compression should be calculated from the installed geometry rather than inferred from the compound name. The relevant inputs are gasket free thickness, flange closing distance, groove depth, hardness, surface flatness, and bolt preload [S3]. EPDM formulations can be advantageous when flange flatness is poor or available bolt load is limited because their compliance can help the gasket conform to the sealing area [S3].
EPDM and FKM Comparison for Bolted Joints
EPDM and FKM should be compared by service envelope, mechanical behavior, installation tolerance, and joint-design consequences rather than by pressure class alone. The service media, exact temperature profile, flange facing, surface finish, and available bolt load must all be verified before the material is specified [S5].
For a typical static sheet gasket, EPDM offers greater compliance and forgiving installation than FKM. Its usual compression target is 25–40%, with less than 10–15% leaving a risk of unsealed surface irregularities and more than about 50% risking permanent deformation without adequate recovery [S3].
FKM, also known as Viton in many commercial contexts, is suited to demanding thermal and chemical conditions, but it is not a universal substitute for a compliant EPDM joint. That value is not a universal FKM rating because compound, temperature, thickness, hardness, and bolt load remain governing inputs [S4].
The explicit comparison is therefore: EPDM is favored for compliant sealing over imperfect flange surfaces and constrained bolt load, with a normal 25–40% compression target [S3]. FKM is favored where chemical compatibility and elevated-temperature resistance control the selection, with greater sensitivity to accurate compression and sustained seating stress. Flexible graphite has notably low creep relaxation and can provide effective sealability under load once placed [S2], making it an important benchmark when relaxation-driven loss of contact stress dominates.
Flange Conditions That Decide the Result

A gasket cannot remain properly compressed if the joint geometry cannot supply the required force. Gasketed joints require smooth flange surfaces, adequate bolt load, and sufficient flange flatness [S6]. Flange alignment and parallel faces must therefore be inspected before gasket installation, not after a leak appears.
For EPDM, the joint should be tightened so that the completed gasket thickness produces the selected compression percentage, rather than tightening to a generic torque value. That value was a discussion calculation, not a standardized installation instruction, and it does not replace a documented torque-and-tension procedure.
Sheet gaskets must also match the flange facing. RTJ rings require RTJ groove flanges, while spiral-wound and kammprofile constructions are generally more suitable than soft sheet gaskets where pressure and temperature cycling are significant [S5]. For low-pressure water, HVAC, and utility service, full-face or ring-style elastomer gaskets may be appropriate when chemical compatibility is confirmed [S5].
Plain EPDM sheet gaskets are described for Class 150 and Class 300 water flanges at approximately 16–25 bar, depending on hardness, thickness, and bolt load [S8]. This range should not be transferred directly to steam, hydrocarbons, strong oxidizers, or concentrated chemicals. The lower limit among media compatibility, temperature, pressure, and mechanical load governs the selection [S4].
Temperature, Media, and Chemical Constraints
EPDM is normally selected for water, steam, and many chemical services where the elastomer's temperature envelope and chemical compatibility are acceptable. A compound that seals a cool water line can still be unsuitable for hot oil, steam condensate, or a solvent exposure, so the exact fluid, concentration, temperature, and cycling frequency must be checked [S5].
FKM is normally considered when elevated-temperature resistance and broad hydrocarbon or chemical compatibility are required. It should not be selected from the family name alone because compounding, exposure time, and temperature affect swelling, aging, and recovery. For steam, hot oil, or cyclic thermal service, gasket construction with suitable recovery behavior should be evaluated [S5].
Thermal cycling is the practical concern in both materials. The joint may seal at ambient installation, then lose contact stress after heat-up because the gasket relaxes and the bolt load drops [S4]. If the application requires resistance to creep relaxation and cold flow, particularly with PTFE-based materials at elevated temperature or low seating stress, that behavior must be included in the joint design [S5].
Installation Controls That Limit Relaxation

Controlled compression is the first line of defense against relaxation-related leakage. Measure gasket thickness before assembly, use a specified closing distance or controlled bolt-tension method, and verify that the final compression falls within the gasket supplier's range. For solid EPDM, 25–40% is the normal design target, not a nominal value that can be ignored [S3].
Uniform preload matters as much as total load. An even bolt pattern supports uniform gasket compression and reduces the risk of local gaps, distortion, or leakage [S7]. Flange rotation, damaged gasket seating surfaces, debris, and a misaligned gasket can produce local over-compression even when the average calculated compression is correct.
For dissimilar metals, differential thermal expansion can alter flange spacing and bolt load. Control of temperature ramps, joint geometry, and the gasket's compression-set behavior is therefore part of the material decision, not a secondary installation issue. The material guide for EPDM rubber provides a broader compound and service context, while the handbook entry for fluororubber covers the FKM family used in high-performance elastomeric sealing.
A practical EPDM specification can also be coordinated with hardness selection, as discussed in Specify EPDM Flange Gaskets at 60–70 Shore A. Hardness changes the force needed to reach a target compression, so it must be linked to gasket dimensions, flange stiffness, and available bolt load rather than copied as a standalone material requirement.
Procurement and Qualification Checklist
Specify the compound, gasket style, dimensions, hardness, free thickness, flange facing, service media, temperature range, pressure, and required compression in the purchase specification. The same material family can contain different fillers, cure systems, and service ratings, so approval should reference a supplier's grade datasheet and test data rather than the words EPDM or FKM alone [S5].
Request evidence that is relevant to installed behavior: ASTM D395 compression-set data for the applicable test temperature and duration, dimensional tolerances, and a recommended compression range. For EPDM, verify that the selected compound can support the planned thermal cycling and pressure range. For FKM, verify compatibility with the exact media and concentration and define the permissible temperature and pressure envelope for the specific grade [S4].
Before installation, record the flange class, face type, bolt count and size, target tightening method, gasket thickness, and initial closing distance. After assembly, verify compression and gasket centering. The final selection is defensible when the minimum of the chemical, thermal, pressure, and mechanical limits remains within the grade's documented capability.
Use EPDM where compliant static sealing, imperfect flange flatness, or limited preload makes installation tolerance decisive. Use FKM where the process envelope, especially temperature and chemical exposure, justifies it, and qualify the loss of contact stress under sustained load. Track final gasket thickness and bolt-load changes through the first heat-up as the two practical checks on relaxation.