Aluminum Alloy 7178

Aluminum alloy 7178 is a wrought alloy of the 7xxx series in which zinc is the main alloying element, with magnesium and copper added to make it harden by heat treatment. It was registered in 1954 and was made for aircraft structures, where it served as sheet, plate and extrusion in parts that had to be both light and strong. Its registered limits give it more zinc, magnesium and copper than alloy 7075, the 7xxx alloy most buyers know, and that is the source of both its strength and its limitations. Today it is met mostly as sustainment stock for older airframes and as a line on a legacy drawing, so the buyer's task is less to exploit the alloy than to buy it correctly and to know when another material is the better choice.

The alloy is easy to define and harder to place. Its composition is fixed by registration, so two certificates that both say 7178 describe material with the same limits. What is not fixed is the strength a designer may count on: the handbook that once published design values for 7178 removed it, and the current edition treats it as an obsolete alloy that is highly susceptible to stress corrosion cracking. The figures that remain in the public record are test results from particular lots, published by government laboratories. This page sets out what is registered, what is published and what a purchaser has to settle with a supplier, so that a request for quotation for 7178 states the alloy, the temper, the form, the specification and the basis of the strength values in the same sentence.

Bar chart of the registered composition limits of aluminum alloy 7178 by weight percent: ranges for zinc 6.3 to 7.3, magnesium 2.4 to 3.1, copper 1.6 to 2.4 and chromium 0.18 to 0.28, and maximum limits of 0.50 for iron, 0.40 for silicon, 0.30 for manganese, 0.20 for titanium and 0.05 each for other elements.

Diagram: SpecForge original bar chart, drawn for this page from the Aluminum Association registration record.

Where the buying decision concentrates: in the temper and in the basis of the strength values. A 7178 purchase today is usually a repeat of a purchase made decades ago, and the questions that matter are whether the material matches the registered limits, whether it carries the temper the drawing calls for, what minimum properties the supplier will guarantee, and which approved source of design values the part will be sized against. The answers sit in four documents: the registration record, the specification on the drawing, the mill certificate and the allowable basis the design authority accepts.

Chapter 1 / 06

What Aluminum Alloy 7178 Is and How It Works

Aluminum alloy 7178 is a wrought alloy, which means it is shaped by rolling, extruding or forging rather than by casting. A casting alloy is melted and poured with a casting ladle in a casting plant, or injected into a die casting die in an aluminum die casting machine; wrought 7178 never is. The four-figure name follows the international designation system for wrought aluminum. The first digit names the alloy group by the element present in the greatest mean percentage, and the group 7xxx is the zinc group. The registration record lists 7178 as registered in 1954 by the United States, in the same year as alloy 7075, and keeps it among the active wrought alloys: it appears in the table of calculated nominal densities for active alloys and not in the table of inactive designations. The aluminum alloy family is wide; this page is about the one alloy.

Strength comes from heat treatment and from the three elements that make the alloy respond to it. In solution heat treatment the product is heated to a suitable temperature, held long enough for the alloying constituents to enter into solid solution, and cooled fast enough to hold them there. Artificial aging then makes the zinc, magnesium and copper come out of solution as fine precipitates that obstruct the planes along which the metal would deform. The registered limits of 7178 contain more of all three elements than those of 7075: zinc 6.3 to 7.3 percent against 5.1 to 6.1, magnesium 2.4 to 3.1 against 2.1 to 2.9, and copper 1.6 to 2.4 against 1.2 to 2.0, each by weight. The limits on silicon, iron, manganese, chromium and titanium are the same in the two alloys.

The full registered composition is short enough to read from a certificate. Silicon is limited to 0.40 percent, iron to 0.50, manganese to 0.30 and titanium to 0.20, and chromium is held to a range of 0.18 to 0.28 percent. Unlisted metallic elements, grouped as others, may reach 0.05 percent each and 0.15 percent in total, and aluminum makes up the remainder. Two conventions matter when a certificate is checked. A single figure is a maximum unless it is shown as a range or a minimum, and an analytical result is rounded to the last place of the limit before it is judged against that limit. The former ISO chemical designation for the same composition is AlZn7MgCu. The registration also marks 7178 as the original alloy of its family; the later designation 7278, registered in 1981, adjusts its limits for particular products.

Two physical properties are needed for most design work, and they carry different weights of authority. The nominal density is 0.102 lb/in3 (2.83 x 10^3 kg/m3). The registration record computes this value from the composition rather than measuring it by a weight method, rounds it to a stated number of decimal places, and warns that it should not be written into a specification as an engineering requirement; its proper use is estimating the weight per unit area or per unit length. The elastic modulus is a measured quantity. In the government test programs the modulus of 7178-T6 lots ranged from 66.9 to 69.7 GN/m2 (9.7 x 10^6 to 10.1 x 10^6 psi), and the extrusion taken from a transport aircraft wing measured 69.0 GN/m2 (10.0 x 10^3 ksi).

The published strength figures are averages of the lots that were tested. One program tested 7178-T6 sheet in three thicknesses, 1.3 mm (0.05 in.), 4.1 mm (0.16 in.) and 6.4 mm (0.25 in.). Ultimate tensile strength averaged 608, 624 and 622 MN/m2 (88.2, 90.5 and 90.2 ksi), yield strength 564, 586 and 593 MN/m2 (81.8, 85.0 and 86.0 ksi), and elongation 12.7, 12.8 and 13.0 percent, from three to six tests per thickness. A second program cut specimens from a machined 7178-T6 extrusion that had served 6,385 flight-hours in the upper wing surface of the center wing box of a transport airplane; it measured 657 MN/m2 (95.3 ksi) ultimate, 605 MN/m2 (87.8 ksi) yield and 8.9 percent elongation. None of these numbers is a specification minimum.

Strength alone did not decide where the alloy could be used; toughness and cracking did. In the same test program the fracture toughness of the 6.4 mm (0.25 in.) material was about two-thirds of that of the thinner gages, and fatigue cracks generally grew somewhat faster in the thicker gages than in the thinnest. At a nominal thickness of 5.1 mm (0.20 in.), cracks in 7075-T6 and 7178-T6 grew to a given length in about the same number of cycles, but the toughness of 7075-T6 was about 20 percent higher. Intermittent bursts of crack growth appeared inside specimens 4.1 mm (0.16 in.) thick and thicker. The T6 temper also has the lower resistance to stress corrosion cracking, which is the property that later ended the alloy's use in new designs.

Chapter 2 / 06

Aluminum Alloy 7178 Types and Structural Variants

The forms in which the alloy was specified can be read from the handbook record. When the design handbook listed the alloy as obsolete it named bare sheet and plate in five tempers, T6, T62, T651, T76 and T7651, produced to the federal specifications QQ-A-250/14 and QQ-A-250/21. Extrusion was another form: the wing material studied after service was a 7178-T6 extrusion from which the test specimens were machined. Sheet is the thin product, bent or formed to shape, and plate the thick one, machined from solid; the thickness at which the name changes from sheet to plate is a matter for the product specification and not for the alloy. A buyer who meets 7178 today meets it as one of these forms, and the form belongs in the order as much as the alloy does.

The temper names follow a system that is the same for all aluminum alloys, and each digit carries a meaning. T6 means solution heat-treated and artificially aged, with no cold work after the solution treatment other than straightening whose effect is not recognized in the property limits. T62 means solution heat-treated from the annealed or as-fabricated condition and artificially aged; it is also applied when the user heat treats the material from any temper and reaches the properties of the temper. T651 adds stress relief by stretching: plate is stretched 1.5 to 3 percent permanent set after the solution treatment and receives no further straightening, which lowers the residual stresses that would otherwise add to the applied stress in thick plate.

The T76 tempers belong to the T7 family, in which the product is aged beyond the point of maximum strength on purpose, to control a characteristic other than strength. That characteristic is corrosion. The last revision of the government design handbook states the ranking in plain terms for alloys of the same series: the T76-type temper gives good exfoliation resistance and higher stress corrosion resistance than the T6-type tempers of 7075 and 7178, and the T73-type temper provides the highest resistance to stress corrosion. The handbook that followed it adds that the tempers with the lowest resistance to stress corrosion cracking also have the lowest resistance to exfoliation, and that tempers which improve one improve the other. For 7178 the choice between T6 and T76 was therefore a trade of strength for corrosion resistance.

Two kinds of neighbor are worth distinguishing from 7178. The first is the alloy it resembles. Alloy 7075 shares the limits on silicon, iron, manganese, chromium and titanium and differs in having less zinc, magnesium and copper; it remained in the design handbook, and it is the reference material in the tests quoted in this page. Alloy 7079, another high-strength zinc alloy, shared the fate of 7178: the handbook record lists it as an obsolete alloy highly susceptible to stress corrosion cracking. The second kind of neighbor is the later designation inside the family, 7278 and 7278A, which are separate registered compositions and not other names for 7178. A certificate that gives either is not a certificate for 7178.

What 7178 is not is as useful to know. It is not a casting alloy: the melting furnace, the casting ladle and the die casting die play no part in its production. It is not an additive manufacturing material, and a certificate for metal powder made by gas atomization describes a different product with its own oxygen and particle size limits. It is not one of the architectural alloys either; the metal of an aluminum ladder or an aluminum veneer panel is chosen for extrudability and for the look of its anodic film, not for strength. A cold forged heat treated aluminum forging is a formed part made from a soft-temper alloy and then treated, and it is covered on its own page. In a bill of materials 7178 sits with parts of other families, an alloy steel fastener or a titanium alloy fitting, and each keeps its own specification.

Surface protection is part of the material decision for every 7xxx alloy, and for 7178 it is not optional. The practice is to limit exposure of the bare surface in the temper that is susceptible. The Air Force standard that governs launch vehicles calls for maximum use of those alloys, heat treatments and coatings which minimize susceptibility to pitting and to general, intergranular and stress corrosion. For sheet that can mean a pure aluminum or aluminum-zinc cladding rolled onto the core, so that the cladding corrodes first and protects the core; for machined parts it means an industrial coating system with a conversion coating beneath the paint. The thickness of such a film is checked with a coating thickness gauge at the points where the film is thinnest.

Chapter 3 / 06

Key Specification Parameters and Standards

A purchase order for 7178 has to say four things: the alloy, the temper, the form and the document that defines acceptance. The alloy and temper are written under the system defined in ANSI H35.1, the American National Standard for alloy and temper designations, which the registration record cites as the system it follows. The form is covered by a product specification: for sheet and plate the common one is ASTM B209, the standard specification for aluminum and aluminum-alloy sheet and plate, which the standards body lists as active. The historical record names the federal specifications QQ-A-250/14 and QQ-A-250/21 for 7178 sheet and plate. A present-day order should name the specification that the drawing or the design authority requires and not assume that an old number can still be ordered to without an agreed equivalent.

Strength values are where 7178 differs most from an alloy in current use, and the buyer needs to know which kind of number is under discussion. A design allowable is a statistical minimum that a procuring or certifying agency has accepted. The handbook that publishes such values for aerospace alloys, MMPDS, which continues the government handbook MIL-HDBK-5, no longer carries any for 7178: its table of obsolete alloys lists the bare sheet and plate tempers and gives the basis for removal as an obsolete alloy that is highly susceptible to stress corrosion cracking. The launch-vehicle standard of the Air Force spells out the consequence: strength allowables come from the handbook, from government material specifications or from other widely accepted industry specifications, and where the data are not there, contractor allowables developed in accordance with the handbook may be used with approval.

What a mill certificate shows is narrower: the heat analysis against the registered limits, the temper, the form and the results of the mechanical tests required by the product specification. Those tests are made on specimens from the lot on a tensile testing machine, and they report what that lot did. The averages published for the lots tested by the government laboratories, 608 to 624 MN/m2 (88.2 to 90.5 ksi) ultimate and 564 to 593 MN/m2 (81.8 to 86.0 ksi) yield for T6 sheet, show the level a specification minimum will sit below. The service study found the properties of the wing material still above the B design values of the handbook revision of its day after 6,385 flight-hours, which is evidence about that material and not a guarantee about a new lot.

ParameterRegistered or published valueWhat it decides
Zinc, magnesium, copper6.3 to 7.3, 2.4 to 3.1 and 1.6 to 2.4 percent by weightThe alloying content that gives strength; first check on a certificate
Chromium0.18 to 0.28 percent by weightGrain structure control; a range, not a maximum
Silicon, iron, manganese, titanium0.40, 0.50, 0.30 and 0.20 percent maximumImpurity limits; identical in alloy 7075
Other elements0.05 percent each, 0.15 percent totalUnlisted metallic elements; aluminum is the remainder
Nominal density0.102 lb/in3 (2.83 x 10^3 kg/m3), computedWeight estimates; not an acceptance limit
T6 temperSolution heat-treated and artificially agedHighest strength, lowest stress-corrosion resistance
T651 temperPlate stretched 1.5 to 3 percent after solution treatmentLower residual stress in thick plate
T76 and T7651 tempersOveraged beyond maximum strengthBetter exfoliation and stress-corrosion behavior
Ultimate tensile strength608 to 624 MN/m2 (88.2 to 90.5 ksi), T6 lots testedReference level only; agree minimum values with the supplier
Yield strength564 to 593 MN/m2 (81.8 to 86.0 ksi), T6 lots testedBasis of stress sizing once an allowable is agreed
Elongation12.7 to 13.0 percent, T6 lots testedFormability and ductility indication
Elastic modulus66.9 to 69.7 GN/m2 (9.7 x 10^6 to 10.1 x 10^6 psi)Deflection and stiffness calculations
Design allowablesNone in the current MMPDSAn approved alternative basis is required
Chapter 4 / 06

Selection and Duty Calculations

The calculations that follow are the ones an engineer makes when 7178 appears on a drawing. Each uses only the registered and published figures of this page, and each is an illustration of method: for a real part the allowable must come from a basis the design authority has accepted.

The first question is whether the alloy may be used at all for the part in hand. The Air Force standard for expendable launch vehicles states that aluminum alloys 2020-T6, 7079-T6 and 7178-T6 shall not be used for structural applications unless specifically approved, and it prohibits any alloy with a stress corrosion threshold below 25 ksi in any grain direction. A commercial or industrial design will not be bound by that document, but it states the professional consensus in a form that a materials review board can cite. For a new design the practical answer is to choose an alloy that still carries handbook data. For a legacy part the answer is to keep 7178 where the drawing calls for it and to document the basis of every value used.

Strength sizing starts from an allowable, not from a published average. To show the arithmetic, take a bracket cut from 6.4 mm (0.25 in.) plate that must carry 150 kN. Suppose the design authority accepts a working stress of 0.8 times the yield strength measured for the tested lots of that thickness, 593 MN/m2 (86.0 ksi), which gives 474 MN/m2. Since one MN/m2 is one newton per square millimeter, the bracket needs a cross-section of 150,000 N divided by 474 N/mm2, about 316 mm2, which in 6.4 mm plate is a width of 49 mm. The 0.8 factor is an illustration. A real factor of safety is set by the design rules in force, and the starting strength must be a guaranteed minimum, because half of a normal production can be expected to fall below the average.

Weight and stiffness are the second pair of calculations, and both use the physical properties. Take a plate 1 m by 2 m and 6.4 mm (0.25 in.) thick. Its volume is 0.0128 m3, and at the nominal density of 2.83 x 10^3 kg/m3 it weighs 36 kg. Another aluminum alloy of the same size weighs almost the same and is just as stiff, so a part sized by stiffness gains nothing from 7178. Against a steel plate it gains in strength per unit of weight but hardly in stiffness per unit of weight, because the two ratios are close. The gain from 7178 is in strength per unit of weight, which is why its uses were parts sized by strength. When a drawing is revised to a titanium alloy or a nickel alloy for toughness reasons, the stiffness calculation has to be made again.

Damage tolerance calculations take their inputs from the fracture data, and for 7178 those inputs depend on thickness. The tested sheet lost about one third of its fracture toughness between the thin gages and 6.4 mm (0.25 in.), so a toughness measured on thin sheet overstates the toughness of thick plate. At the same nominal thickness 7075-T6 had about 20 percent higher toughness while cracks grew at about the same rate, so a crack that would be tolerated in 7075-T6 may reach critical length earlier in 7178-T6 at the same stress. Bursts of crack growth in material 4.1 mm (0.16 in.) and thicker add scatter to the growth rate. The conservative course is to use toughness data measured on the product form and thickness in question and to set the inspection interval from that data.

Stress corrosion is checked against the sustained tensile stress, not against the peak load. The launch-vehicle standard asks that assembly stresses be kept below the stress corrosion threshold for the alloy, temper and grain-flow direction, and it allows thin 7075-T6 and similar sheet only where the short transverse loads are below acceptable stress corrosion limits. A bolt that squeezes a 7178 lug, an interference-fit bushing or a tightly clamped joint can hold a tensile stress in the short transverse direction for years, and in the T6 temper that is the condition in which cracking develops. Two checks follow. The first is to lower the sustained stress by relief holes, by larger clamp areas or by a stress-relieved temper such as T651. The second is to keep water out of the joint and to break the dissimilar-metal couple formed with carbon steel or copper material, which drives pitting at the joint.

Situation in the designWhat it means for 7178Decision
New structural design in T6Restricted by the launch-vehicle standard; no current design allowablesChoose an alloy that still carries handbook data
Legacy drawing or sustainmentMaterial and temper are fixed by the original designBuy to the drawing; record the allowable basis used
Tensile stress held for long periodsT6 tempers are highly susceptible to stress corrosion crackingLower the sustained stress; use a stress-relieved or overaged temper
Thick plate in a fracture-critical partToughness falls by about one third at 6.4 mm (0.25 in.)Use toughness data from the form and thickness; size from damage tolerance
Part sized by stiffness, not strengthModulus is that of aluminum, 66.9 to 69.7 GN/m2No stiffness gain over other aluminum alloys
Outdoor or marine exposurePitting, exfoliation and galvanic attack on unprotected surfacesClad or coat; isolate from carbon steel and copper
Material to be heat treated by the userT62 applies to material treated from the annealed or as-fabricated conditionSpecify the route and certify the properties achieved
Supplier offers an equivalent7278 and 7278A are different registered compositionsCheck the certificate against the 7178 limits
Strength data needed for certificationPublished figures are lot averagesQualify by test or use approved contractor allowables
Chapter 5 / 06

Installation, Maintenance, and Typical Failure Modes

A 7178 part that reaches the shop is checked before it is made, watched while it is assembled and inspected while it is in service. The sequence below follows the documents already named: the registration record, the product specification and the corrosion rules of the launch-vehicle standard.

Receiving inspection starts with the certificate and ends, where the order requires it, with a test. The certificate should carry the heat number, the chemical analysis, the temper, the form and the mechanical test results, and the analysis is checked against the registered limits after it has been rounded in the prescribed way. The mechanical tests are tensile tests, made on a tensile testing machine on specimens taken from the lot in the directions the specification names. A portable hardness tester gives a quick indication of condition but is not an acceptance test for strength. An eddy current tester reading electrical conductivity is a useful check that the material is in the temper stated, because conductivity moves with the condition of the precipitates.

Internal and surface discontinuities are the second check. Plate that will be machined into a critical part is commonly scanned with an ultrasonic flaw detector before any metal is removed, because a void or a rolled-in inclusion found after machining has already cost the machining time; industrial x ray examination belongs to castings and welds and is rarely needed for wrought plate. Machined and suspected parts can be checked for surface-breaking cracks with a dye penetrant kit, a method that needs no instrument beyond the kit itself and shows cracks at holes and fillets where stress concentrates. Surface finish is a separate matter and a simple one: 7178 machines to a good finish with sharp tools on conventional machine tools, the measured finish is read with a surface roughness tester, and the finish matters mainly where a part is fatigue-critical.

Assembly is where corrosion protection is won or lost. Coated or clad sheet must not be handled with tools that cut through the film, and where the coating is damaged in forming or in riveting the damaged area is restored before the assembly is closed. Contact with dissimilar metals is the other risk. Carbon steel fasteners corrode and cause galvanic attack on the aluminum around them unless they are plated, and even stainless steel fasteners are set in sealant or with an isolating washer in aggressive locations; copper material such as a bus bar or a plumbing fitting should never touch the alloy bare. The thickness of the restored film is verified with a coating thickness gauge, and the reading is checked against the minimum the drawing specifies.

In service the failures that matter start locally, while the bulk of the metal keeps its properties. The service study supports the second half of that statement: after 6,385 flight-hours the wing material showed no significant difference from new material in notched and unnotched fatigue strength, in fatigue crack growth rate, in fracture toughness or in tensile properties. Cracks in an aging airframe therefore come from stress concentrations, from corrosion at joints and from wear at holes rather than from a general weakening of the alloy. A fatigue crack will start at a hole or a corner and grow in the direction the load dictates; a stress corrosion crack will follow the grain structure in the short transverse direction under a sustained bolt load; exfoliation will lift layers of metal at an edge. Each has its inspection method and its own repair.

Maintenance decisions on 7178 parts are mostly decisions about when to stop repairing. A cracked part can be reinforced, reamed and bushed or replaced, and the choice rests on the fracture data for its thickness and on the inspection interval the data allow. Re-heat-treating a finished part in a heat treatment furnace to recover properties is rarely sound, because the quench distorts a thin part and the aging of a thick section depends on the time it took to cool. Where a part is retired, the material is recovered as scrap of value only if it is kept separate from other alloy families: mixed 7xxx scrap is downgraded, and the zinc and copper it carries would pass into whatever is melted with it. The drawing, the certificate and the repair record follow the part until it is scrapped.

Failure modeHow it showsWhat to do
Stress corrosion crackingCracks along the grain in the short transverse direction under a sustained tensile stressLower the assembly stress; protect the surface; change the temper or the alloy
Exfoliation corrosionLayers of metal lifting at edges and around fastener headsRestore the coating; keep water out of joints; inspect on schedule
Fatigue crackingCracks from holes and corners; faster growth in thicker gagesInspect by interval; size the part by damage tolerance
Low toughness in thick sectionsFracture at a lower stress than thin sheet would tolerateUse toughness data for the actual thickness; limit the thickness
Property shortfallTensile results below the values assumed in designSpecify minimum values; never size from lot averages
Wrong condition after user heat treatmentConductivity or hardness outside the expected bandTreat to a qualified procedure and retest the lot
Galvanic corrosionWhite or gray powder around steel or copper contactsPlated fasteners; sealant or isolating washers; restore coating
Lost traceabilityNo heat number or certificate with the materialQuarantine the stock until it is certified or requalify it by test
Chapter 6 / 06

Industry Applications and Procurement Checks

The application that shaped 7178 was the aircraft airframe. The government reports that measured it describe 7075-T6 and 7178-T6 as materials in frequent use in aircraft construction, and the alloy served in the upper wing surface of a military transport's center wing box, a location sized by strength under compression. Its uses were therefore plate, sheet and extrusions in wings, fuselage frames and fittings. In later designs the alloy gave way to others, and composite structure made from carbon fiber took over the upper wing skins of many airliners. What remains is a fleet of older aircraft and the spare parts they need, which is where a buyer meets 7178 now.

Buying it now is a matter of sources and documents rather than of price. Stock is held by service centers and by mills that roll or extrude to order, and a quotation should state whether the material is prime, with a mill certificate, or surplus with a certificate that may be incomplete. The specification on the drawing decides what is acceptable: where it names a number that is no longer current, the design authority has to agree the document that replaces it before the order is placed. Where strength values are needed for a repair or a re-evaluation, the basis of those values has to be agreed at the same time. The two questions are asked together because neither a certificate alone nor an allowable alone makes a part airworthy.

Industrial uses outside aviation are few, and a buyer outside aerospace who is offered 7178 should ask why. Its properties are those of an aerospace alloy bought for strength per unit of weight, and an industrial part in aluminum is more often made from an alloy that can be welded or formed without the corrosion precautions that 7178 needs. Its working is that of any aluminum alloy: it is sawn, milled and drilled on the same machine tools, and a dimensional check of the finished part is made with ordinary instruments. It has no place in a building, where the aluminum veneer panel and similar products are extruded from other alloys. In a bill of materials it belongs beside the other aerospace alloys, not beside the general engineering parts in alloy steel or carbon steel made in the same shop.

For an inquiry, state the alloy by its registered designation, 7178, and the temper and the product form, whether sheet, plate or extrusion, with the thickness and the dimensions. Name the specification and the revision the drawing requires, or ask the supplier which current document covers 7178 in that form and have the replacement agreed in writing. Ask for the mill certificate with the heat number and the full chemical analysis, and check each element against the registered limits, remembering that a single figure is a maximum. Ask for the mechanical test results for the lot, with the direction of testing and the number of tests, and state the minimum values the lot must meet instead of quoting a published average. Ask whether the material was heat treated by the mill or will be treated after forming, and state the temper that applies in each case. Where design values are needed, ask the design authority which allowable basis it accepts and record the answer with the order. Finally, ask how the surface is protected, whether the material is clad, coated or bare, and have any damaged coating restored before the part is assembled.

FAQ

What is aluminum alloy 7178?

Aluminum alloy 7178 is a wrought alloy of the 7xxx series, the group in which zinc is the main alloying element, with magnesium and copper added so that it hardens by heat treatment. It was registered in 1954 and was made for aircraft structures as sheet, plate and extrusion. Its registered limits contain more zinc, magnesium and copper than alloy 7075, which gives it higher strength and lower toughness and stress corrosion resistance. It is no longer common in new designs and is bought today mainly as material for older airframes and for parts on legacy drawings.

What is the chemical composition of aluminum alloy 7178?

The registered limits, by weight, are zinc 6.3 to 7.3 percent, magnesium 2.4 to 3.1 percent, copper 1.6 to 2.4 percent and chromium 0.18 to 0.28 percent. Silicon is limited to 0.40 percent, iron to 0.50, manganese to 0.30 and titanium to 0.20, other metallic elements may reach 0.05 percent each and 0.15 percent in total, and aluminum makes up the remainder. The former ISO chemical designation for the same composition is AlZn7MgCu. The designations 7278 and 7278A are separate registered compositions and must not be supplied as 7178.

What tempers does aluminum alloy 7178 come in?

The handbook record names five tempers for bare sheet and plate: T6, T62, T651, T76 and T7651. T6 is solution heat-treated and artificially aged and gives the highest strength. T62 applies when the user heat treats the material and ages it to the same properties. T651 is plate stretched 1.5 to 3 percent after the solution treatment to lower residual stress. T76 and T7651 are overaged tempers that give up some strength for better resistance to exfoliation and stress corrosion cracking. The temper belongs on the order with the alloy, because the same plate in two tempers is two different materials in service.

How strong is aluminum alloy 7178?

The published figures are averages of the lots tested by government laboratories, not guaranteed minima. For T6 sheet 1.3 to 6.4 mm (0.05 to 0.25 in.) thick, ultimate tensile strength averaged 608 to 624 MN/m2 (88.2 to 90.5 ksi), yield strength 564 to 593 MN/m2 (81.8 to 86.0 ksi), with 12.7 to 13.0 percent elongation. A T6 extrusion from a transport aircraft wing, tested after 6,385 flight-hours, gave 657 MN/m2 (95.3 ksi) ultimate and 605 MN/m2 (87.8 ksi) yield. The elastic modulus was 66.9 to 69.7 GN/m2. For design, use a minimum value agreed with the supplier or an allowable from an approved basis, never a published average.

Why is aluminum alloy 7178-T6 restricted in structural design?

Because the T6 temper is highly susceptible to stress corrosion cracking. The handbook that publishes aerospace design allowables lists 7178 sheet and plate among its obsolete alloys on that ground and publishes no design values for it. The T6-type tempers of 7178 are the reference against which the handbook describes tempers with higher stress corrosion resistance. The Air Force standard for expendable launch vehicles bars 7178-T6 from structural applications unless a specific approval is given. New designs therefore use other alloys; 7178-T6 is kept where a legacy drawing requires it, with its sustained stresses held low and its surface protected.

What should be checked when aluminum alloy 7178 is received?

Check the certificate first: the heat number, the full chemical analysis against the registered limits, the temper, the product form and the mechanical test results for the lot. A single figure in the limits is a maximum, and an analysis is rounded before it is judged. Where the order requires tests, tensile specimens are tested from the lot, and plate for a critical part is scanned for internal discontinuities before machining. A hardness tester or an electrical conductivity reading is a quick check of condition, not an acceptance test. Material without a certificate is kept apart until it is certified or requalified. The surface protection is inspected for damage, which is restored before the part goes into assembly.

Is aluminum alloy 7178 the same alloy as 7075?

No. The two are separate registered alloys, although both date from 1954 and share the limits on silicon, iron, manganese, chromium and titanium. Alloy 7178 has more zinc, magnesium and copper, and in the government tests 7075-T6 showed about 20 percent higher fracture toughness at the same nominal thickness, with about the same rate of fatigue crack growth. Alloy 7075 kept its place in the design handbook and in new designs; 7178 did not. For a new part, 7075 is the more usual choice and is supplied with current design data. For a part designed in 7178, the alloy should be changed only through the design authority that owns the drawing.

Sources

  1. Aluminum Association: Teal Sheets, International Alloy Designations and Chemical Composition Limits (PDF)
  2. NASA TN D-7173: Specimen thickness effect on fatigue crack growth and fracture toughness of 7075-T6 and 7178-T6 (PDF)
  3. NASA TM X-3165: Effect of service usage on tensile, fatigue and fracture properties of 7075-T6 and 7178-T6 (PDF)
  4. US Air Force SMC-S-011: Parts, materials and processes control program for expendable launch vehicles (PDF)
  5. MIL-HDBK-5J, Chapter 3.7: 7000 series wrought alloys
  6. ASTM: B209 Standard Specification for Aluminum and Aluminum-Alloy Sheet and Plate
Ask SpecForge AI