Cold-Forged Heat-Treated Aluminum Forging

A cold-forged heat-treated aluminum forging is an aluminum alloy part built in two stages. A slug, a blank sheared from wire or a sawn length of rod is first shaped at room temperature: headed, extruded, coined, pressed or sized in a steel die set. The shaped part is then precipitation heat treated, which means it is solution treated, quenched and aged to the temper written on the drawing. The route is chosen for parts made in large numbers with close tolerances, thin walls and little scrap: rivets, thin-walled housings, airbag and seat-belt components and heat sinks. The alloy family is described on the aluminum alloy page; this page is about the part and the route that gives it its properties.

The page is written for the engineer who has to specify such a part, qualify a supplier and accept its lots. It covers what the cold work and the heat treatment each do, which alloy families and tempers are used before and after forming, how far aluminum can be pushed at room temperature, the specification and test values a buyer states, distortion and residual stress, anodizing, lot acceptance and the ways the route fails. Process values come from a forging design guide, a cold-forming guide, an impact extrusion maker's technical page, the government handbook of aluminum alloy design data and an FAA advisory circular. Where a figure is general practice rather than a published value, it is stated as typical.

Process route diagram for a cold-forged, heat-treated aluminum forging: an aluminum slug or billet in a soft temper goes by cold heading, impact extrusion, coining and cold pressing, or cold sizing, then through cleaning and solution heat treatment, quench, straightening, artificial aging, finishing and inspection.

Diagram: SpecForge original schematic, drawn for this page.

Five things decide a cold-forged heat-treated aluminum forging purchase. First the alloy and the temper, which fix strength, corrosion behavior and how much the part can be formed cold. Second the process route, whether heading, impact extrusion, coining or cold sizing, because each suits a different shape and press. Third the heat treatment, since solution treating, quenching and aging set the final properties and the distortion. Fourth the inspection the lot must pass: tension, hardness and conductivity evidence that the treatment was done. Fifth the quantity, because hard tooling and fast presses pay back only at volume. Get those five stated and the part repeats.

Chapter 1 / 06

What a Cold-Forged Heat-Treated Aluminum Forging Is and How It Works

The definition has two halves and both matter. Cold forging, in the words of the forging design guide listed in the sources, is performed at or near room temperature, and work hardening occurs; hot processes run where work hardening is diminished or absent. Heat treatment adds the second half: the shaped part is solution treated so that its alloying elements dissolve, quenched rapidly enough to hold them in solution, and aged so that they come out again as a fine precipitate. The finished part is a wrought structure whose grain flow was shaped by the die, not a cast one, and its final strength is set by the aging step rather than by the press stroke that shaped it.

What the cold work does is easiest to see by watching the stock. The punch must push the metal past its yield strength before it flows at all, and once it flows the alloy strain hardens: the impact extrusion maker's page attributes this to dislocation movement in the aluminum lattice and notes that strength rises while ductility falls. The cold-forming guide adds the consequence that matters to the tool engineer: yield strength climbs faster than tensile strength, so the window between the two narrows at every station, and a part worked too far in one hit fractures. Severe shapes are therefore split across several dies, and the stock is bought soft so that the window starts wide.

What the heat treatment does is less obvious. A buyer might expect the cold work to survive into the finished part as extra strength, and it does not. The government handbook that publishes design data for aluminum alloys warns that cold working before solution heat treatment can cause recrystallization or grain growth during the treatment, and that the resulting strength, particularly yield strength, may fall below the specified minimums. It advises testing the part after forming, heat treating and straightening rather than trusting the stock certificate. The cold work leaves its trace mainly as grain size and grain flow; the strength of the finished temper comes from aging, which the forging guide places at 120 to 175 degrees Celsius (250 to 350 degrees Fahrenheit).

The working parts are few and each has one job. The stock arrives as coiled wire or rod, sawn slugs or preformed blanks; the impact extrusion maker reports that most of its slugs are round or rectangular and has feedstock checked by ultrasonic testing when a customer asks, the task of an ultrasonic flaw detector. The die set is cut from tool die steel, and its inner surface becomes the surface of the part. Knuckle-joint mechanical presses are standard for impact extrusion, reaching 330 strokes per minute on small parts, and a screw press or a servo press serves where ram speed must be controlled. Aluminum forms no scale, so lubrication is essential to keep it from seizing and galling against bare die steel.

Physically the metal is redistributed, not removed. Upsetting shortens a length of blank and thickens it; extrusion pushes it through a smaller opening or back up along the punch, and in every case the volume of the blank stays constant. No chips are made, so the heading guide puts scrap at 1 to 3 percent of the blank mass. The grains are elongated and follow the outline of the part instead of being cut through by a tool, which is why the fillet under a headed shoulder is tougher than one turned from bar. Nothing melts and nothing shrinks on cooling, so there is no porosity; the extrusion maker supplies parts for storing pressure media on that basis.

The boundaries deserve one sentence each. A hot die forging is shaped at high temperature, so press loads are lower and more deformation is possible, but it needs draft and its tolerances and surface are coarser. A die-cast part belongs to another family: a die casting machine or a gravity die casting machine fills a steel die casting die with liquid alloy, which makes thin walls cheaply but leaves no grain flow, and machining can open shrinkage cavities in the metal. A part pressed from metal powder and sintered is porous by nature. A part machined from bar cuts through the grain and turns most of the blank into chips. The cold-forged, heat-treated part suits quantities that pay for its tooling.

Chapter 2 / 06

Cold-Forged Heat-Treated Aluminum Forging Types and Process Variants

Cold heading is the oldest variant and still the one made in the largest numbers. A blank sheared from wire is struck on its end inside a die so that the metal mushrooms into a head, a collar or a spline; the cold-forming guide defines heading as a forging operation without heat, usually combined with sizing, piercing and trimming. Its limit is geometric, and the same guide, written for steel and specialty alloys, gives the rule of thumb: in one blow a solid-die header can upset about 2.25 wire diameters, and a longer unsupported length buckles and folds into a cold shut; two blows raise the limit to 4.5 diameters. Rivets are the classic output, and the rivet alloys driven in aircraft, 2117, 2017 and 2024, are headed from wire rod drawn to cold-heading quality.

Forward and backward extrusion make the shapes that heading cannot. In forward extrusion the blank is pushed into a smaller die opening and leaves it longer and thinner; in backward extrusion a punch presses into the blank and the metal flows up around the punch, which yields sleeves, nuts, tubes and cups. The guide's rules distinguish open and trapped extrusion: open extrusion is limited to a 30 percent reduction of area in one blow at an extrusion angle of 30 degrees or less, while trapped extrusion, with the blank fully contained, reaches 75 percent. Impact extrusion is the backward-extrusion variant run at speed on a knuckle-joint press: one stroke turns a slug into a thin-walled cup.

Coining, cold pressing and cold sizing are the finishing variants, and they are where the close tolerances come from. In coining the surface of a preform is squeezed hard against a fine die face so that every feature fills; the load is high because the metal has little room to move. Cold pressing closes a preform in a single die so that its outline and bore reach final size. Cold sizing irons a bore or a face back into tolerance after heat treatment has moved the part. The government handbook records the same idea among its tempers: a T54 temper is a die forging stress relieved by restriking it cold in the finish die.

Alloy choice follows the series. Pure 1xxx metal and the 6xxx alloys dominate impact extrusion; the maker's page names the 1000 and 6000 groups as its most frequent stock, and the anodizers council rates the 6xxx series as having an excellent response to anodizing. Pure-metal heat sinks are credited with up to 30 percent higher thermal conductivity than cast ones. The 3xxx and 5xxx alloys are not heat treatable and are used in strain-hardened tempers. The 2xxx alloys headed into rivets are strong, hard and high in copper, and they gain their strength from aging. The 7xxx alloys, the strongest of all, are mostly forged hot, because the series is sensitive to how fast it is deformed.

The temper before forming and the temper after it are separate decisions. Annealed O stock is the softest starting point and the usual choice for severe forming. The freshly quenched state is the other: the FAA circular notes that some alloys may be formed over appreciably smaller radii immediately after quenching, and the handbook recommends forming in that state or at elevated temperature to limit residual stress. The outcome follows from the sequence. Solution treating and natural aging give T4; recognized cold work between quench and natural aging gives T3; artificial aging after solution treatment gives T6; and cold work followed by artificial aging gives T8, a temper the extrusion maker also offers.

Where the route sits economically is fixed by tooling and quantity. Cold tools cost five to ten times what equivalent hot impression dies cost, yet their tool life is much longer, so the route suits very high quantities. The cold-forming guide puts the threshold at about 5,000 parts for a shape that a one- or two-blow header can make and at 25,000 to 30,000 pieces for a part that needs several dies and development work. Weight is the other limit: commercial cold forgings typically weigh under 23 kg (50 lb). Outside those limits a machined part or a hot forging is the sounder buy.

Chapter 3 / 06

Key Specification Parameters and Standards

A specification for this part is short, and every line of it binds the supplier. It states the alloy and the temper, the product specification, the minimum mechanical properties and the grain directions they apply in, the tolerances and surface finish on as-forged and on machined faces, the finish, and the tests each lot must pass. For die forgings the metric specification ASTM B247M, the SI companion of ASTM B247, calls for chemical analysis, tension and hardness tests, heat treatment, heat-treat response and stress corrosion testing. Heading stock is bought to ASTM B316, wire and rod suitable for cold heading, with designations assigned under ANSI H35.1. The parameters that recur are listed with their usual values.

Mechanical properties are stated as minimums; the government handbook gives reference floors for three often ordered alloys. For 6061-T6 die forgings up to 4.000 in (102 mm) thick it lists 262 MPa (38,000 psi) ultimate and 241 MPa (35,000 psi) yield, with 7 percent elongation lengthwise. For 2014-T6 die forgings up to 1.000 in (25 mm) thick the figures are 448 MPa (65,000 psi) and 386 MPa (56,000 psi), with 6 percent elongation; for 7075-T6, 517 MPa (75,000 psi) and 441 MPa (64,000 psi), with 7 percent. Hardness is the shop-floor number: with a 500 kg load and a 10 mm ball, the FAA circular gives Brinell 95 for 6061-T6, 135 for 2014-T6 and for 7075-T6, 120 for 2024-T4 and 65 for 6061-T4.

The remaining parameters describe shape and service. Impact-extruded walls go down to less than 0.5 mm (0.02 in) without loss of properties, and because nothing shrinks on cooling the shape tolerances match the tool. Corrosion behavior follows composition and aging cycle: the 2xxx alloys, with several percent of copper, are more prone to atmospheric corrosion, pitting and galvanic attack than 7xxx alloys low in copper, and 2014 and 7075 in T6-type tempers are listed as open to stress corrosion cracking. The handbook permits a sustained tensile stress of 50 to 75 percent of minimum yield only for the resistant tempers. The forging guide uses aluminum forgings up to about 150 degrees Celsius (300 degrees Fahrenheit), and strength falls off fastest between 212 and 400 degrees Fahrenheit (100 and 204 degrees Celsius).

ParameterTypical value or requirementWhat it decides
Alloy families cold formed1xxx and 6xxx for extrusion; 2xxx rivet alloys for headingSource of strength: cold work, aging or both
Aging temperature120 to 175 degrees Celsius (250 to 350 degrees Fahrenheit)Strength against corrosion resistance
6061-T6 die forging, ultimate and yield262 MPa (38,000 psi); 241 MPa (35,000 psi)Design stress, general-purpose alloy
2014-T6 die forging, ultimate and yield448 MPa (65,000 psi); 386 MPa (56,000 psi)Design stress, copper-bearing alloy
7075-T6 die forging, ultimate and yield517 MPa (75,000 psi); 441 MPa (64,000 psi)Highest strength, smallest corrosion margin
Brinell hardness, 500 kg load, 10 mm ball95 for 6061-T6; 135 for 2014-T6 and 7075-T6Shop check that aging was done
Minimum wall, impact extrusionless than 0.5 mm (0.02 in)Weight and internal space
Impact-extruded size, one maker's rangeup to 500 mm (19.7 in) long, 150 mm (5.9 in) diameterWhether a housing fits the process
Upset in one blow2.25 wire diametersNumber of heading stations
Decorative anodic coatingunder 0.4 mil (10 microns)Corrosion protection and appearance
Chapter 4 / 06

Selection and Duty Calculations

Selecting a cold-forged heat-treated aluminum forging comes down to fixing five things in order: the alloy, the stock temper, the forming route, the final temper and the inspection. Each choice narrows the next, and a few short calculations show whether a proposed shape can be made at all.

Start from the duty, not from the alloy. A part that must carry load, resist weather and look good is a 6xxx job: 6061 forgings carry 262 MPa (38,000 psi) ultimate at the handbook floor, the series responds well to anodizing, and the forging guide lists 6061-T6 among its commonly forged alloys. A part that needs the highest strength and will be coated or kept indoors points to 2014 or 7075, and the temper question follows at once, because the handbook lists both in T6-type tempers among the combinations susceptible to stress corrosion cracking. Where a sustained tensile stress cannot be designed out, an overaged T7x temper buys resistance at a cost in strength. Pure 1xxx metal is chosen for conductivity and formability.

The geometry then picks the process. A blank with a head or a collar on a shaft of one diameter is a heading job, within the upset limit of 2.25 diameters per blow. A cup, a can or a housing closed at one end is an impact extrusion job, and the thin wall it permits is the reason battery, motor and sensor housings are made that way. A part whose bore or face must hold a tight tolerance after heat treatment is coined or sized, cold in the finish die or in a separate stroke. The features to avoid are the same whatever the route: sharp internal corners, holes deep in proportion to their diameter, and large steps between diameters, since each concentrates metal flow and raises the tool load.

The first calculation is the blank. Volume is conserved, so the blank equals the part in volume, and the heading guide notes that headed weight can be held within 1 percent, or 0.2 percent with precise cut-off. The heading ratio, blank length divided by wire diameter, follows the guide's example: a blank 5 in (127 mm) long of 0.5 in (12.7 mm) wire is 10 diameters long, of which 1 in (25 mm) can be upset in one blow and 2 in (51 mm) in two, while 3 in (76 mm) is 6 diameters and cannot be controlled. For extrusion the check is reduction of area: a blank of 1.00 sq in (645 mm2) extruded to 0.75 sq in (484 mm2) is a 25 percent reduction, inside the 30 percent limit for open extrusion.

The third calculation is press load, and it decides whether the shape is feasible. Metal flows only when the stress at the punch face exceeds the yield strength of the stock, and that yield strength rises as the part strain hardens from station to station; the cold-forming guide also finds that forming speed and part geometry change the effective strength. No simple formula gives the peak load of a real part, so toolmakers rely on simulation and on trial strokes with the force read by a load cell on the press. The press is then chosen with margin: one impact extrusion shop runs presses from 150 to 1200 tons and reports a largest knuckle-joint press of 2,000 tons.

The fourth calculation sizes the section from the property floor. A link in 6061-T6 that must carry 50 kN in tension at the handbook yield needs at least 50,000 N divided by 241 N per square millimeter, about 207 mm2 (0.32 sq in) of section, before any allowance for stress concentration or corrosion. Two cautions go with the arithmetic. The handbook values apply to the thickness at the time of heat treatment, and when forgings are machined before heat treatment the as-forged thickness may be no more than twice the treated thickness. Properties of forgings are also stated for at least two directions, so a part loaded across the grain must be sized on the lower figure.

Decision factorOptionsWhat tips the choice
Stock temperO annealed, or freshly quenchedSeverity of forming; grain growth risk
Final temperT4; T6; T8; overaged T7xStrength against stress corrosion
Forming routeHeading; impact extrusion; coining; cold sizingShaft with a head, cup, detailed face, tight bore
Annual quantityabout 5,000 simple; 25,000 to 30,000 complexTooling payback against station count
Part weight and wallunder 23 kg (50 lb); walls to 0.5 mm (0.02 in)Press rating; fit to the process
Residual stress relief1 to 3 percent compression; restrike in finish dieMachining movement; sustained tensile stress
Corrosion protectionDecorative anodize under 0.4 mil (10 microns); hardcoat 1.0 to 5.0 mils2xxx and 7xxx alloys, outdoor exposure, wear
Lot acceptanceHardness; tension per lot; conductivityPart criticality; where heat treatment was done
Chapter 5 / 06

Heat Treatment, Finishing, and Typical Failure Modes

Forming is over in seconds. Heat treatment, straightening and finishing decide what the part is finally worth, and each of those steps carries its own failure. The inspection that follows each step is chosen for the failure that step can cause, and the numbered sequence keeps the steps in that order.

Solution treatment puts the alloying elements into solid solution, and three things can go wrong in it. A furnace that runs too hot melts low-melting constituents, the eutectic melting that the heat-treatment practice ASTM B918 lists among its tests. A load that was cold worked, as every cold-forged part was, can recrystallize or grow grain and lose yield strength. A furnace that is not uniform gives varied properties across the rack. The practice therefore requires furnace temperature uniformity and calibration, with racking, spacing and cleanliness. In the shop that means the heat treatment furnace is surveyed, its temperature controller is calibrated, and a load thermocouple or other temperature sensor travels with the parts. For wrought alloys in aerospace work its scope points to AMS2772.

Quenching must be fast enough to hold the constituents in solution, and it is where distortion and residual stress begin. The FAA circular asks for quenching as rapidly as possible after the furnace, prefers cold water, and allows hot or boiling water or an air blast for bulky sections such as forgings when quenching stresses must be reduced. Straightening belongs immediately after the quench, while the part is soft and before aging locks the stresses in. Aging at 120 to 175 degrees Celsius (250 to 350 degrees Fahrenheit) brings the strength up; continuing past the peak overages the part to a T7x temper, trading some strength for better stress corrosion and toughness. The rivet alloys 2017 and 2024 are damaged by any later heating above 212 degrees Fahrenheit (100 degrees Celsius), including the baking of primer.

Distortion and residual stress are one problem seen at two different times. The quench locks a stress pattern into the part and straightening adds a pattern of its own; the handbook names solution heat treatment, straightening, forming, fit-up and clamping as stress sources that have caused stress corrosion failures. The registered remedies are mechanical: stretching or compressing after the quench, with die forgings stretched 1 to 5 percent permanent set and compression set at 1 to 3 percent, or restriking cold in the finish die. Aging itself changes dimensions very little, in most wrought alloys less than half the growth seen in alloy 2219. Where low stress must be proven, hole drilling with a strain gauge rosette gives a number, and a CMM check before and after machine tools cut the stressed skin shows whether the relief worked.

Finishing starts with cleaning and usually ends with anodizing. Heading lubricant is removed with a vapor degreaser or an industrial solvent, the parts are deoxidized to strip the natural oxide, and an etch in weak caustic soda gives a matte surface. The anodizers council's bulletin is emphatic that the anodic film is transparent and hides nothing, so forging marks, die wear and scratches show through, and a surface roughness tester on the as-forged face predicts the gloss. Thickness is a class decision: protective and decorative films are under 0.4 mil (10 microns), architectural class II runs 0.4 to 0.7 mil, class I starts at 0.7 mil, and hardcoat runs 1.0 to 5.0 mils where wear matters. Copper-bearing 2xxx alloys anodize with difficulty, 6xxx alloys respond excellently and 7xxx alloys come out mottled gray.

Inspection closes the route. An inspection lot, in the words of the cold-heading wire specification, is an identifiable quantity of one mill form, alloy, temper and nominal diameter traceable to its heat-treat lots, and the certificate should say so. A tension test on a tensile testing machine proves the temper, and hardness, read on a bench hardness tester or a portable hardness analyzer on a large part, is the daily check. The FAA circular limits what hardness can tell: it separates annealed from heat-treated material of a known alloy and leaves a small pit, so it is kept off joint faces, fatigue-critical parts and load-bearing areas. Conductivity, read with an eddy current tester, is the check the circular names when heat damage is suspected. Dimensions go to a CMM or an articulated arm CMM.

  1. Degrease the parts and rack them with spacing so that the quench reaches every surface, with the furnace survey and calibration current.
  2. Solution treat at the temperature and time in the part's heat-treatment instruction; reject any sign of eutectic melting.
  3. Quench as soon as the load leaves the furnace, in cold water or, for bulky forgings, in hot water or an air blast.
  4. Straighten at once, while the alloy is soft, and stress relieve by stretching, compression or restrike if the drawing calls for it.
  5. Age at the specified temperature and time, then read hardness across the lot before releasing it for machining.
Failure modeWhere it comes fromCheck and remedy
Cracking or cold shut in formingUpset beyond 2.25 diameters in one blow; formability used upSplit the upset across stations; form soft or freshly quenched
Low yield strength after treatmentRecrystallization from cold work before solution treatmentTest the finished part; form after solution treating
Eutectic melting and porosityFurnace too hot or unevenSurveyed, calibrated furnace; porosity test
Movement in machiningQuench and straightening stress released by cuttingStress relieve by 1 to 3 percent compression or restrike
Soft or overaged partAging off cycle; 2017 or 2024 reheated above 212 degrees Fahrenheit (100 degrees Celsius)Hardness and tension per lot; control later baking
Stress corrosion crackingSustained tensile stress on T6-type 2xxx or 7xxx alloyT7x temper, stress relief, coating, lower assembly stress
Pitting and galvanic attackBare 2xxx alloy, or contact with less active metalsAnodize; isolate the contact or change alloy
Dimensions drifting with die wearTool wear widening tolerancesCheck die wear on tight runs; rework the tool
Chapter 6 / 06

Industry Applications and Procurement Checks

Road vehicles take the largest share of the cold-formed aluminum parts made today. The impact extrusion maker lists battery and motor housings, heat sinks for power electronics, sensor and camera housings, air spring components, steering and brake elements, damper components, airbag housings and seat-belt tensioners. Its pure-metal heat sinks, credited with up to 30 percent higher thermal conductivity than cast ones, serve LED headlights and vehicle electronics. Aerospace, automotive, truck, military and sporting uses are the older market for heat-treated forgings, and aircraft rivets in 2117, 2017 and 2024 remain the classic headed part. Anywhere a thin-walled, sound, light part is needed in tens of thousands is a candidate.

Buyers give the same reasons across these industries. Material is saved because nothing is cut away, and heading scrap runs at 1 to 3 percent of the blank. Soundness is assured in the sense that matters to a pressure housing: no blowholes, no shrinkage, a homogeneous microstructure. Accuracy comes with the tool, since the part takes the tool's dimensions with no shrinkage on cooling and, in a flashless die, no trim edge to dress. Against a hot forging the extrusion maker claims less weight, a better surface for coating, tighter tolerances and lower energy use; against machining, a material saving that grows with quantity. Small parts run at up to 330 strokes per minute on a knuckle-joint press.

Cost and lead time are driven by tooling and by the number of operations, not by the metal. Cold dies cost several times hot dies, so the first order carries die engineering, trial strokes and heat treatment of the tools; the impact extrusion maker keeps tool cost down by building its tools in its own shop. Each extra station adds a die and a transfer step. After forming, every lot passes through cleaning, solution treatment, quench, straightening and aging, with stress relief and anodizing where the drawing asks, and each of those is a batch with its own schedule; an outside heat treater or anodizer adds a supplier and a queue. Lead time grows with the number of processes more than with the number of pieces.

A purchase order for a cold-forged heat-treated aluminum forging should state on the drawing: the alloy and the temper, for example 6061-T6, with the cold process route named; the material specification, ASTM B247M for forgings or ASTM B316 for heading stock, and the heat-treatment practice, ASTM B918 or its aerospace equivalent, if the supplier treats in house; the minimum tensile, yield and elongation values and the grain directions they apply in; whether hardness alone accepts the lot or tension, conductivity or stress corrosion tests are required; the tolerances on as-forged and on machined faces; any stress relief required and any limit on machining before heat treatment; the finish, with anodic coating thickness and color, or an industrial coating over a thin anodic film where the part is painted; marking, with a laser marker rather than a stamp on thin walls, and lot traceability including the heat-treat lot number on the certificate; and the first-article inspection report. Ask the supplier which tempers it forms in, where its thickness limit at heat treatment falls, and what its largest press allows.

FAQ

What is a cold-forged heat-treated aluminum forging?

It is an aluminum alloy part shaped at room temperature in a steel die set and then strengthened by heat treatment. The shaping may be cold heading, impact extrusion, coining, cold pressing or cold sizing. The heat treatment is a precipitation treatment: the part is solution treated, quenched and aged to a temper such as T4, T6 or T8. Typical parts are rivets, thin-walled housings for batteries, motors and sensors, airbag and seat-belt components, and heat sinks. The buyer receives a sound part with grain flow following its outline, close tolerances, little scrap and thin walls, provided the quantity pays for the tooling.

Which aluminum alloys and tempers are used?

Pure 1xxx metal and the 6xxx alloys, 6061 above all, are the usual stock for impact extrusion, and the 2xxx rivet alloys 2117, 2017 and 2024 are headed into fasteners. The 3xxx and 5xxx alloys are not heat treatable and are used in strain-hardened tempers, while 2014 and 7075 are the high-strength forging alloys. Stock is formed either in the annealed O temper or in the soft, freshly quenched state. The resulting temper follows from the sequence: natural aging gives T4, cold work after quenching gives T3 or T8, and artificial aging gives T6. Where stress corrosion is a concern, an overaged T7x temper is specified instead.

Which specifications matter most?

Three cover most purchases. ASTM B247M, the metric companion of ASTM B247, covers die, hand and rolled ring forgings and calls for chemical analysis, tension and hardness tests, heat treatment and stress corrosion testing. ASTM B316 covers wire and rod for cold heading. ASTM B918 is the practice for heat treating wrought aluminum alloys for general purposes and points to AMS2772 for aerospace work. Design values for forgings are published in the government's aluminum alloy handbook, MIL-HDBK-5. The drawing should also state the lot traceability and the test report required.

How does cold forging differ from hot forging and die casting?

A hot forging is shaped with the alloy heated, so the press needs less force and larger deformations are possible, but the part needs draft, cools with some loss of accuracy and has a coarser surface. Cold forging work hardens the metal, which raises press loads and tooling cost, five to ten times that of hot dies, and returns tighter tolerances, no draft and a better surface. A die-cast part comes from a different family: a die casting machine fills a steel die with liquid alloy, which allows thin walls at low cost but leaves no grain flow and can hide shrinkage cavities that machining later opens.

What does heat treatment change in a cold-forged part?

Almost everything that matters mechanically. The cold work does not remain as strength: solution treating can recrystallize the grain, and the handbook warns that yield strength may fall below minimums when a heavily worked part is judged on its stock certificate alone. Strength is rebuilt by aging at 120 to 175 degrees Celsius (250 to 350 degrees Fahrenheit), which precipitates the alloying elements. The quench and any straightening leave residual stress that can distort the part in later machining, so straightening is done at once and stress relief by stretching, compression or restriking is applied where specified. Hardness follows the temper: 6061 rises from 65 Brinell in T4 to 95 in T6.

How is a heat-treated lot checked and accepted?

By a certificate tied to an identifiable lot and by tests made on that lot. The specification for cold-heading wire defines an inspection lot as one mill form, alloy, temper and diameter traceable to its heat-treat lots, and the certificate should carry those references. A tension test proves the temper. Brinell hardness is the routine check, read on a bench hardness tester or a portable hardness analyzer; it separates heat-treated from annealed material of a known alloy but leaves a small pit. Electrical conductivity, measured with an eddy current tester, is the check named when heat damage is suspected. An anodic coating, if there is one, is measured for thickness.

What drives cost and lead time?

Tooling and the number of operations. Cold dies cost five to ten times hot forging dies, which is why the route suits quantities of about 5,000 simple parts or 25,000 to 30,000 complex ones; commercial cold forgings also weigh under 23 kg (50 lb). Each station in a heading or extrusion sequence adds a die and a transfer, and each step after forming, cleaning, solution treatment, quench, straightening, aging, stress relief and anodizing, is a scheduled batch. Working the other way are die life, scrap of only 1 to 3 percent, and fast presses that reach 330 strokes per minute on small parts.

Sources

  1. MIL-HDBK-5H: Metallic Materials and Elements for Aerospace Vehicle Structures, 1 December 1998 (PDF)
  2. FAA AC 43.13-1B: Acceptable Methods, Techniques, and Practices, Aircraft Inspection and Repair (PDF)
  3. Forging Industry Association: Product Design Guide for Forging (PDF)
  4. Neuman Aluminium: Impact extrusion technology page
  5. Carpenter Technology: Heading Hints, a Guide to Cold Forming Specialty Alloys (PDF)
  6. ASTM: B247M Standard Specification for Aluminum and Aluminum-Alloy Die Forgings, Hand Forgings, and Rolled Ring Forgings (Metric)