For 3-inch steel, Victor cutting tip size 4 is charted at 40–50 psig cutting oxygen, 6–17 psig preheat oxygen, and 5–10 psig acetylene [S1][S4].
The controlling reference is the chart for the exact tip system, torch configuration, fuel gas, hose arrangement, and material thickness. Without that documentation, a multi-hole oxy-fuel cutting tip below 1½ inches of steel has a fallback setting of 40 psig oxygen and 10 psig acetylene, but injector-style cutting tips do not follow that rule [S3].
Why Tip Number Is Not Enough
Tip-size numbers can correspond to different operating pressures in different charts, and [S2] notes that tip-size numbers vary among manufacturers and therefore lists welding orifices by number-drill size [S2]. For 3-inch steel, Victor cutting tip size 4 is charted at 40–50 psig cutting oxygen, 6–17 psig preheat oxygen, and 5–10 psig acetylene [S1][S4].
Tip numbers also vary between manufacturers, so a numerical size should not be transferred automatically to an unrelated product. One pressure reference addresses this by presenting cutting tips through number-drill orifice sizes rather than relying only on tip numbers [S2]. The practical hierarchy is manufacturer chart, torch owner’s manual, then a documented fallback rule. Manufacturer data should remain first because it accounts for the details that govern flame behavior and gas consumption [S3].
For multi-hole oxy-acetylene cutting tips below 1½ inches of steel, the emergency fallback is 10 psig acetylene and 40 psig oxygen. If manufacturer settings are unavailable for multi-hole oxy-acetylene cutting of steel less than 1½ inches thick, set the acetylene regulator to 10 psig and the oxygen regulator to 40 psig [S3]. These values are general settings, not a substitute for a manufacturer chart [S3].
Read the Chart by Tip Geometry
The pressure value belongs to a defined geometry. One-piece cutting tips may use a straight oxygen bore intended for approximately 40–60 psi in hand-cutting service, while a divergent-bore design requires a different operating approach [S6]. A user must identify whether the consumable is a cutting tip, a welding nozzle, a multi-flame heating nozzle, or a single-hole brazing or welding tip before selecting a pressure.
For Victor acetylene cutting tips, size 000 uses 20–25 psig cutting oxygen for 1/8-inch steel, size 2 uses 35–40 psig for 1 inch, size 4 uses 40–50 psig for 3 inches, and size 8 uses 45–55 psig for 12 inches [S1][S4]. These are chart values for the stated 1-101 or 3-101 torch series, not universal values for every tip marked with the same number.
The comparison is straightforward: welding tip size 4 is charted at 5–10 psig oxygen, while acetylene cutting tip size 4 is charted at 40–50 psig cutting oxygen. Number-drill size distinguishes the former as 49, or 0.073 inch, but the cutting chart identifies size 4 by application and metal thickness rather than by a single welding-nozzle drill value [S1][S4].
Match Oxygen Setting to Torch and Hose
The chart value must be reconciled with how the torch meters oxygen. A three-hose cutting torch has separate cutting-oxygen and preheat-oxygen controls, while a two-hose torch derives preheat from the cutting-oxygen supply. The Victor chart therefore states that its separate preheat-oxygen range applies only to three-hose machine cutting torches [S4].
Hose length and diameter also affect the pressure available at the tip. The recommended pressures are measured with gas flowing and may require regulator adjustment to accommodate hose size and length [S5]. For Victor acetylene tips size 6 and larger, the chart specifies pressures measured at the regulator using a 25-foot by 3/8-inch hose and recommends an appropriately rated torch with the same 3/8-inch hose size [S4].
Flashback arrestors create another correction. The Victor documentation states that torches with flashback arrestors can require up to 25% more pressure as tip size increases, with a maximum acetylene pressure of 15 psi [S4]. This is a specific equipment condition, not a blanket instruction to raise every regulator. Operators should apply it only where the chart and torch documentation identify the arrestor configuration.
Set and Verify Flowing Pressure
Regulator settings are not the final proof because line loss can make torch pressure differ from panel pressure.
A direct check of the selected Victor cutting ranges shows how sharply the setting changes with workpiece size. Size 000 is charted at 20–25 psig cutting oxygen for 1/8-inch steel, size 1 at 30–35 psig for 3/4 inch, size 3 at 40–45 psig for 2 inches, and size 5 at 45–55 psig for 4 to 5 inches [S1][S4]. The same charts also pair these with cutting speeds of 20–30 ipm, 17–21 ipm, 12–15 ipm, and 8–11 ipm for those respective entries [S4].
Material thickness is not the only operating variable. Fuel-gas choice alters the chart. The Victor acetylene cutting-tip chart lists tip size 4 for 3-inch steel at 40–50 psig cutting oxygen, 6–17 psig preheat oxygen, and 5–10 psig acetylene [S4]. The fuel-gas value and chart family must therefore remain explicit in the work instruction.
Apply Limits for Heaters, Injectors, and Cylinders
Multi-flame heating nozzles require their own table rather than a cutting-tip rule. Victor MFA size 4 uses 8–12 psig oxygen and 6–10 psig acetylene, while the supplied excerpt also lists size 6 at 8–12 psig oxygen and 10–15 psig acetylene [S1][S4]. Badger explicitly states that there is no rule of thumb for rosebud heating tips because incorrect settings can cause flashback or meltdown [S3].
Injector-style cutting torches are another exclusion. The 40 psig oxygen and 10 psig acetylene fallback applies to multi-hole oxy-acetylene cutting tips below 1½ inches, not injector-style equipment [S3]. Injector torches mix fuel and oxygen upstream, so applying a conventional multi-hole chart or generic cutting rule can produce the wrong operating condition.
Supply capacity must be checked as well. The Victor charts state that withdrawal from an individual acetylene cylinder should not exceed one-seventh of the cylinder contents per hour; additional demand requires a manifold system of adequate capacity [S1][S4]. For Victor size 12 welding nozzles, the chart lists 18–28 psig oxygen, 12–15 psig acetylene, and acetylene consumption of 80–160 SCFH, while size 15 calls for 50–60 psig oxygen and 90–220 SCFH [S1][S4].
Build a Defensible Selection Record
The correct oxygen pressure can be verified by recording six items: tip marking, tip function, fuel gas, torch model and hose configuration, metal thickness, and the required flowing pressure. The selection record should also state the chart revision or manufacturer document used, because the available Victor acetylene chart contains a 2011 publication marker and a 25-foot hose measurement basis [S4].
Operator checks should distinguish the two principal pressures in a three-hose cutting system: cutting oxygen for the kerf and preheat oxygen for the initial ignition zone. The acetylene size 3 entry is 40–45 psig cutting oxygen, 5–14 psig preheat oxygen, and 4–9 psig acetylene for 2-inch steel, while size 6 is 45–55 psig cutting oxygen, 10–22 psig preheat oxygen, and 7–13 psig acetylene for 6-inch steel [S1].
A related cutting-consumable comparison for choosing the correct cutting tip for 2-inch steel plate helps narrow the tip family, but the final oxygen setting still comes from the chart for that exact tip and torch system. For the Victor 1-101 and 3-101 series, 2-inch steel corresponds to tip size 3 at 40–45 psig cutting oxygen and 4–9 psig acetylene [S1][S4].
Before starting a cut, confirm that the selected chart matches the physical consumable, set the regulators within its stated ranges, purge and light the torch under the manufacturer procedure, and verify pressure at the torch while gas flows. Then compare the flame and cut condition with the charted operating range, escalating to the torch manufacturer if the required pressure cannot be achieved.